镁铬砖一般是由烧结镁砂和耐火级铬矿为原料生产的,耐火晶粒间为硅酸盐结合,国内所说的镁铬砖,一般是指烧成的普通镁铬砖,简称镁铬砖。
镁铬砖的耐火度大于2000℃,荷重软化温度一般在1550℃以上,高温体积稳定性好,耐急冷急热性比镁砖强。再结合镁铬砖
|
Behaviors |
||||
Magnesia Chrome Bricks |
|||||
TY-AMC-40 |
TY-AMC-20 |
TY-AMC-12 |
TY-AMC-8 |
||
Chemical |
MgO % |
35 |
60 |
70 |
70 |
SiO2 % |
1.0 |
1.0 |
2.0 |
2.0 |
|
Cr2O3 % |
40 |
20 |
12 |
8 |
|
显气孔率Apparent Porosity % |
16 |
16 |
18 |
18 |
耐压强度Cold Crushing Strength Mpa |
40 |
40 |
40 |
40 |
荷重软化温度0.2Mpa Refractoriness Under Load T0.6 |
1700 |
1700 |
1650 |
1650 |
体积密度Bulk Density g/cm3 |
3.3 |
3.15 |
3.05 |
3.0 |